Mmiri mmiri ozuzo na-eme ka igwe anaghị agba nchara
Alloy okpomọkụ dị elu
◆0Cr17Ni7Al bụ igwe na-eme ka mmiri ozuzo sie ike nke ejiri Al gbakwunyere, ejiri ya dị ka isi iyi, igwe na-asa akwa, ihe mgbako, wdg.
◆0Cr15Ni7Mo2Al na-eji maka elu-ike containers, akụkụ na structural akụkụ na ụfọdụ corrosion eguzogide chọrọ.
◆Arụmọrụ 0Cr15Ni5Cu4Nb yiri nke 0Cr17Ni4Cu4Nb, mana ọ nwere arụmọrụ n'akụkụ ka mma.
◆0Cr12Mn5Ni4Mo3Al (Gangyan 69111) nwere plasticity dị mma karịa 0Cr15Ni7Mo2Al.
◆0Cr17Ni4Cu4Nb mmiri ozuzo hardening ígwè na Cu agbakwunyere, nke a na-ejikarị na shafts, akụkụ dị ike dị elu nke chọrọ nguzogide corrosion maka akụkụ turbine uzuoku.
◆XM -25 bụ okpomọkụ na elu okpomọkụ na-eguzogide, adabara mmanụ ụgbọala, chemical, aerospace, nuklia ike na ndị ọzọ ọrụ.
Ngwakọta kemịkalụ
Ọkwa | C | Si | Mn | S | P | Cr | Ni | Mo | Cu | Nb | Al | ọzọ |
ọ dịghị ukwuu karịa | ||||||||||||
0Cr17Ni4Cu4Nb | 0.07 | 1 | 1 | 0,035 | 0.03 | 15.5 ruo 17.5 | 3–5 | - | 3–5 | 0.15 ~ 0.45 | - | - |
0Cr17Ni7Al | 0.09 | 1 | 1 | 0,035 | 0.03 | 16–18 | 6.5-7.5 | - | ≤0.5 | - | 0.75 ruo 1.5 | - |
0Cr15Ni7Mo2Al | 0.09 | 1 | 1 | 0,035 | 0.03 | 14–16 | 6.5-7.75 | 2–3 | - | - | 0.75 ruo 1.5 | - |
0Cr15Ni5Cu4Nb | 0.07 | 1 | 1 | 0,035 | 0.03 | 14-15.5 | 3.5-5.5 | - | 2.5-4.5 | 5 *C% ~0.45 | - | - |
0Cr12Mn5Ni4Mo3Al | 0.09 | 0.8 | 4.4-5.3 | 0.03 | 0.03 | 11–12 | 4–5 | 2.7 ruo 3.3 | - | - | 0.5 ~ 1 | - |
XM -25 | 0.05 | 1 | 1 | 0.03 | 0.03 | 14–16 | 5–7 | 0.5 ~ 1 | 1.25 ~ 1.75 | ≥8*C% | - | - |
Alloy onwunwe kacha nta
Ọkwa | steeti | ike tensile RmN/m㎡ | Mpụta Ike Rp0.2N/m㎡ | Mgbatị dị ka% | HRC (HBS) |
0Cr17Ni7Al | siri ike ngwọta 1000 ~ 1100 ℃ ngwa ngwa jụrụ | ≤1030 | ≤380 | ≥20 | ≤229 |
565 ℃ ịka nká | ≥1140 | ≥960 | ≥5 | ≥363 | |
510 ℃ ịka nká | ≥1230 | ≥1030 | ≥4 | ≥388 | |
0Cr17Ni4Cu4Nb | 480 ℃ ịka nká | ≥1310 | ≥1180 | ≥10 | ≥40 |
550 ℃ ịka nká | ≥1060 | ≥1000 | ≥12 | ≥35 | |
580 ℃ ịka nká | ≥1000 | ≥865 | ≥13 | ≥31 | |
620 ℃ ịka nká | ≥930 | ≥325 | ≥16 | ≥28 | |
0Cr15Ni5Cu4Nb | ngwọta siri ike | - | - | - | ≤380 |
565 ℃ ịka nká | ≥1210 | ≥1100 | ≥7 | ≥375 | |
510 ℃ ịka nká | ≥1320 | ≥1210 | ≥6 | ≥388 | |
0Cr12Mn5Ni4Mo3Al | 520 ℃ ịka nká | ≥1520 | ≥1280 | ≥9 | ≥47 |
XM -25 | 560 ℃ ịka nká | ≥1100 | ≥1000 | ≥10 | ≥45 |